ECOLOGICAL INSULATION PLASTER

STANDARD: Conforms to TS EN 998-1

TECHNICAL SPECIFICATIONS

  • Dry unit weight: 300±50 kg/m3

  • Compressive strength: 0,4 N/mm2

  • Heat conductivity factor: ≤ 0.057 W/m.K T1

  • Bond strength: ≤0,2 N/mm2

  • Water vapor permeability: 5,41

  • Reaction to fire: A1

  • Mixing water: 1 kg dry unit/1.5 lt water

  • Workable life and correction time: 30 minutes

  • Hardening period: 36 hours

  • Consumption: 2.65 kg mean for 1 m2 area

  • Capillary absorption: W1

  • Manner of application: Steel trowel / plaster pump

  • Color: Grey / White

  • Packing: 8 kg bag

PREPARATION

  • The surface should be free of anti-sticking agents (mould oil, paint, dust, water) and should be firm.

  • The painted surfaces should be made adsorbent via indentation or paint-cleaning machinery.

  • The surface should be moistened before application.

  • The surface should not have any flaws 

USAGE & APPLICATION

  • 12-14 liters of water is put into a mortar container of at least 50 liters and then 8 kilograms of ecological insulation plaster is poured in.

  • The mortar container that is prepared for mixing should be thoroughly cleaned and at the time of mixing, the edges should be scraped thoroughly with the help of a spud and mixed again.

  • For a homogenous admixture, 500-600 rpm mixers should be used. Mixing time is about 2 minutes.

  • After admixture is rested for approximately 5 minutes, it is mixed again for 1 minutebefore application.

  • If the product starts setting due to delay during application, it should be stirred to obtain application consistency again without water and continued to be applied.

  • The prepared mortar should be used within an hour.  The laths, which will determine the thickness of the ecological insulation plaster, are assembled with appropriate intervals in order for smooth plastering.

  • Ecological insulation plaster, which is prepared, is filled with plaster shovel and spud between laths.

  • 12-14 liters of water with ecological insulation plaster is added to the machine tank 

  • After acquiring a homogenous admixture, it is sprayed between the plaster laths for application.

  • Another method is to feed the machine with the product mixed in the mortar boards and spraying it between the laths.

  • When the product completes thepre shrinkage (without drying), the laths are removed.

  • Then the gaps between the laths are filled with ecological insulation plaster, and they are corrected by a knife gauge and made ready for the finish coat application.